Industry: Municipal Public Drinking Water Company – Basic Sanitation
Operating Conditions: Ambient temperature
Scope:
– Fill the metal to recover the lost surface, reconstruction of edges and corners of the impeller blades.
– Protection against severe wear.
– Protection against corrosion.
– Final finish of the protected surface.
Ceramic for Dredger
November/2024
Flygt N3356 Pump
SEVERE ABRASION:
Material loss on impeller blade edges
Material loss on the wear ring
Ecuador
– Coating with 500 µm thickness
– Recovery offactory dimensions
– Smooth and glossy finish
– Equipment efficiency restored
Proper surface preparation is essentialfor the long-term performance of the coating. The exact requirements for preparation vary depending on the severity of the application, the expected service life, and the initial condition of the substrate.
Prior sanding and grinding of edges and welds
All sharp edges and welds must be ground with an abrasive disc until smooth or with a 3 mm radius to prevent premature failures.
Cleaning and degreasing
Remove contaminants to improve coating adhesion.
Abrasive blasting
Achieve white or near-white finish (SSPC-SP10) with an angular profile between 75–125 µm.
Removal of residues
Carefully remove abrasive residues that may interfere with the application.